Two shops run the same press, the same die insert and the same billet, and one gets three times the service life out of the die. The difference is often not tonnage. It is what happens in the few seconds between two blows.
Heat has to leave the die. Every hot blow pushes heat into the die face. If that heat is not removed, the surface layer softens, the temper is drawn back, and the die begins to wash and gall. Thermal fatigue follows: fine cracks at the radius, then a broken edge. Cool the die too hard and the opposite problem appears — the cold face chills the workpiece, filling becomes difficult and the load on the press rises.
Spray does two jobs. A release agent lowers friction and helps the part leave the cavity; the carrier liquid and the air that follows remove heat. Both functions matter. A shop that sprays just enough to stop sticking, and never checks die temperature, is usually running its dies too hot.
Uniformity beats volume. Nozzles that wet the centre of the die and leave a deep rib dry produce exactly the wear pattern that shows up at the end of die life. Watch the pattern on a cold die with the spray running: every cavity should be wet, and every blow-off path should be clear.
Put the window into the program. A servo screw press runs a programmable cycle, so spray start, spray time, air-blow time and the idle beat before the next billet can be set as data rather than left to operator habit. That is what makes die temperature repeatable from shift to shift. Site material on forging automation describes spray devices working in step with the press cycle and the handling equipment (public site material).
Measure instead of guessing. A contact probe or an infrared gun on the die face before the first blow of a batch, and again after twenty blows, answers the question in a minute. Write the reading next to the spray time in the shift log.
Keep the lines clean. Diluted release agent left in the piping overnight clogs nozzles quietly. Flush at the end of the shift and check nozzle alignment after every die change.
Die life is decided between blows, not on the tonnage plate.
References