郑州华隆专注伺服螺旋压力机

FAQ
FAQ: Why Does Flash Thickness Vary Between the First and the Last Piece?
from:Zhengzhou Haloong Machinery date:2026-11-22

A common complaint in die forging shops: the first piece off a new die set is within tolerance, then flash thickness creeps upward, cavity filling deteriorates, and the weight after trimming drifts. The die is often blamed first, but in most cases the press and the process window explain most of the drift. Three factors deserve checking, in order.

1. Billet consistency. If piece weight or heating temperature varies, the same strike energy deforms the material differently: a cooler or heavier billet leaves thicker flash; a hotter or lighter one fills deeper. Weighing billets and logging furnace discharge temperature turns this from guesswork into data.

2. Energy repeatability. On a friction screw press, the energy delivered to the billet depends on friction wear and on operator judgement, so it drifts through a shift. A servo screw press replaces that chain with closed-loop digital control: strike energy, stroke, speed and position are set as numbers and repeated on every stroke. Site material also notes that the strike parameters — number of blows, force and speed — can be entered as a program, so a multi-blow sequence (lighter blows for venting and positioning, a heavier finishing blow for filling) no longer depends on hand feeling.

3. Die temperature. Cold dies at shift start and warm dies an hour later change flash thickness even when everything else is held constant. A short warm-up schedule and consistent die lubrication narrow the drift without touching the press.

One related point belongs in the comparison. Site material states that the servo drive draws full power only during the forging stroke, with energy consumption reduced by more than 55% compared with a press that keeps consuming idle power, and that stable forming with good anti-deflection behaviour helps extend die service life. For a shop chasing flash consistency, those two characteristics matter as much as the price of the press.

If flash drift persists after billet, energy and die temperature are under control, then — and only then — inspect the die: guide wear, flash land condition and clogged vents are the remaining suspects.

References

  1. Zhengzhou Haloong, News articles on this site: "Why CNC Press Leads High-Precision Taper Bushing Forging", "The forgings look the same, but the quality is very different" (public site material).
  2. GB/T 12362-2016, Steel die forgings — Tolerance and machining allowance (scope covers steel die forgings produced on screw presses).
  3. GB/T 8541-2012, Terminology of forging and stamping.
  4. Forging Handbook (锻压手册), China Machine Press, on the force–energy characteristics of screw presses.
  5. ---